A Comparative Study of Metal Extraction from Spent Catalyst Using Acidithiobacillus ferrooxidans

The recovery of metal values and safe disposal of spent catalyst is gaining interest due to both its hazardous nature and increased regulation associated with disposal methods. Prior to the recovery of the valuable metals, removal of entrained deposits limit the diffusion of lixiviate resulting in low recovery of metals must be taken into consideration. Therefore, petroleum refinery spent catalyst was subjected to acetone washing and roasting at 500oC. The treated samples were investigated for metals bioleaching using Acidithiobacillus ferrooxidans in batch reactors and the leaching efficiencies were compared. It was found out that acetone washed spent catalysts results in better metal recovery compare to roasted spent. About 83% Ni, 20% Al, 50% Mo and 73% V were leached using the acetone washed spent catalyst. In both the cases, Ni, V and Mo was high compared to Al.